Experimental Research on Deep Reduction and Grinding Separation of Low Ti-bearing Vanadium-titanium Magnetite
-
摘要: 对某低钛型钒钛磁铁矿进行深度还原-磨选分离试验,结果表明:还原温度1 050℃,还原时间10 h,是抑制钒还原的临界条件;使用添加剂和延长还原时间能够强化钒钛磁铁矿还原,其中硼砂能够有效促进钒钛磁铁矿还原,硼砂用量3%时,产物金属化率达98.21%,而CaF2在本试验条件下对还原起到抑制作用,弱磁选并深度细磨有利于铁、钒分离。Abstract: Experimental research on deep reduction and grinding separation of a certain low Ti-bearing vanadium-titanium magnetite was conducted.The results show that the critical conditions for inhibiting the reduction of vanadium are reduction at 1 050℃ for 10 h.The reduction of vanadium-titanium magnetite can be enhanced by additives and extension of reduction time.Borax can efficiently promote the reduction of the vanadium-titanium magnetite,and the metallization rate of product reaches 98.21% with 3% borax added.However,inhibitory effects on reduction were observed with CaF2 in the experiments.Low intensity magnetic separation and deep grinding are beneficial to separate Fe and V.
-
Key words:
- vanadium-titanium magnetite /
- deep reduction /
- magnetic separation /
- vanadium extraction
-

计量
- 文章访问数: 84
- HTML全文浏览量: 21
- PDF下载量: 2
- 被引次数: 0