Study on Reducing Soluble Vanadium in the Vanadium-bearing Residue
-
摘要: 针对某钒厂含钒熟料带式过滤机连续浸出过滤生产中残渣可溶钒含量偏高的情况,在实验室进行了熟料粒度、残渣洗水次数、残渣洗水用量、熟料浸泡时间对残渣可溶钒含量影响的模拟及优化试验研究。结果表明:洗水液/固比不低于0.65∶1,残渣洗涤次数不少于3次,浸泡时间大于25 min,可使残渣中可溶钒降至0.12%以下。较改进前(SV0.184%~0.324%),大大提高了钒的回收率,满足了生产要求。Abstract: In view of too high soluble vanadium in the residue during continuous leaching and filtration of vanadium-bearing clinker using the belt filter in a vanadium plant,simulation and optimization experiments were carried out in laboratory to probe into the effects of particle size of clinker,residue washing times,washing water volume and clinker soaking time on soluble vanadium content in the residue.The results show that soluble vanadium can be lowered below 0.12% with the washing liquid to solid ratio no less than 0.65∶1,residue washing times no less than 3 and soaking period more than 25 min.It can be found from experimental results that the vanadium recovery rates are obviously improved compared with previous production(soluble vanadium percentage of 0.184%~0.324%).
-
Key words:
- V2O5 /
- vanadium slag /
- clinker /
- vanadium-bearing residue /
- soluble vanadium(SV) /
- leach
-

计量
- 文章访问数: 60
- HTML全文浏览量: 10
- PDF下载量: 2
- 被引次数: 0